Table 1 Measured viscosity of cell media containing listed polymers

From: Altered motility of Caulobacter Crescentus in viscous and viscoelastic media

PEG 4000 (%)

1.0

2.0

3.0

4.0

5.0

6.0

7.0

8.0

10.0

 

Viscosity (cP)

1.08

1.20

1.44

1.62

1.76

2.06

2.24

2.38

3.03

 

PEG 35000 (%)

0.5

1.0

1.5

2.0

2.5

3.0

3.5

4.0

4.5

5.0

Viscosity (cP)

1.24

1.51

1.88

2.32

2.80

3.32

3.90

4.65

5.30

6.34

PEO 400000 (%)

0.125

0.25

0.375

0.5

1.0

     

Viscosity (cP)

1.59

2.45

3.77

4.88

14.6